Surface Analysis of CLAM steel,EUROFER97 steel and W Irradiated in HT-7 Tokamak

Surface Analysis of CLAM steel,EUROFER97 steel and W Irradiated in HT-7 Tokamak. Qiang Li1,2 Qunying Huang1 Jinnan Yu3 Jiangang Li1 Yican Wu1 Xiaoxiong He1,2 1 Institute of Plasma Physics, Chinese Academy of Sciences, Hefei, Anhui, 230031, CHINA

Download Presentation

Surface Analysis of CLAM steel,EUROFER97 steel and W Irradiated in HT-7 Tokamak

An Image/Link below is provided (as is) to download presentation Download Policy: Content on the Website is provided to you AS IS for your information and personal use and may not be sold / licensed / shared on other websites without getting consent from its author. Content is provided to you AS IS for your information and personal use only. Download presentation by click this link. While downloading, if for some reason you are not able to download a presentation, the publisher may have deleted the file from their server. During download, if you can't get a presentation, the file might be deleted by the publisher.

E N D

Presentation Transcript


  1. Surface Analysis of CLAM steel,EUROFER97 steel and W Irradiated in HT-7 Tokamak Qiang Li1,2 Qunying Huang1 Jinnan Yu3 Jiangang Li1 Yican Wu1 Xiaoxiong He1,2 1 Institute of Plasma Physics, Chinese Academy of Sciences, Hefei, Anhui, 230031, CHINA 2 Hefei University of Science and Technology, Hefei, Anhui, 230039, CHINA 3 China Institute of Atomic Energy, Beijing 102413, CHINA

  2. OUTLINE • About CLAM steel,EUROFER97 steel and W • Experiment procedure Sample Irradiation experiment Surface analysis • Result and discussion Surface morphology Surface composition • conclusion

  3. About CLAM steel,EUROFER97 steel and W • CLAM steel and EUROFER97 steel • low activation ferritic/martensitic steel • Good properties for thermal and neutron irradiation • Being considered as structural material and the first wall material in tokamak

  4. About CLAM steel,EUROFER97 steel and W • W • Refractory high-Z material • High melting ponit,low vapor pressure,good thermal conductivity,high temperture strength and sputtering resistance • Being considered as plasma facing components

  5. Experiment procedure • Sample • Composition of CLAM steel, EUROFER97 steel( wt%) pure multicrystal tungsten(~99.99% wt) • Size:15*7*1.5 mm • All samples were polished and cleaned with acetone and absolute alcohol,and then were dried by hot air.

  6. Experiment procedure • Irradiation experiment • HT-7 tokamak • medium size with limiter, and R=1.22m, a=0.285m, BT≤2.2T • the first wall material is 1Cr18Ni9Ti stainless steel, and the limiter material is graphite coated with SiC

  7. Experiment procedure • Sample shelf and its position in HT-7

  8. Experiment procedure • Plasma average parameters during experiment center: boundary: Ip =125kA ne=1.5*1019m-3 Te =700eV Ti =450eV All samples were irradiated by 802 shots, total irradiation time is about 1200 seconds

  9. Experiment procedure • Surface analysis • Scanning Electron Microscope (SEM) • X-ray Photoelectron Spectroscopy (XPS)

  10. Result and discussion • Surface morphology • CLAM

  11. Result and discussion • EUROFER97

  12. Result and discussion • W

  13. Result and discussion • Number and diameter of blisters • it seemly equal for blister number in CLAM steel surface and EUROFER97 steel surface, and most of blister diameter is less than 1μm • the blisters in W surface are very little ,their diameter are more than 1μm

  14. Result and discussion • Summary • The surface blisters of CLAM steel and EUROFER97 steel are very dense • The blisters seemly range along line in the suface of two kinds of steels • Blisters are observed in the surface of W • Blisters are not observed in the surface of all samples which are far to center plasma

  15. Result and discussion • Surface composition • Si Si peaks are obvious in No.2 samples surface, but it is not obvious for No.1 samples • Other elements No obvious change for No.1 samples and No.2 samples

  16. conclusion • Relative to W,CLAM steel and EUROFER97 steel are more easy to blister when irradiated by plasma • low activation ferritic steel can be used as fisrt wall materials when considering its plasma irradiation resistance ability • If select W as the plasma facing materials,such as divertor armor, more deep researchs must be proceeded